AFM Characterization of Semiconductor Devices

Key takeaways

  • HD-KFM™ distinguishes p- and n-doped regions of an SRAM device (30–50 mV between p-doped areas and n-doped channels, ~300 mV with the n-well) and reveals defective cells invisible in the topography.
  • ResiScope™ on the same area, with the same cantilever, shows which of those cells conduct normally under 1 V bias.
  • On a SiC dopant staircase, ResiScope follows resistance from ~100 Ω to ~1 MΩ across 500 nm steps in one scan.
  • Soft ResiScope™ gives the same values without friction, and follows a VO₂ film from 25 to 50 °C as its current rises from ~100 pA to 6 nA.

CSInstruments · Updated October 2026

Introduction

Electrical characterization at the scale of the device

Semiconductor devices are defined by doping, junctions and interfaces at the scale of tens of nanometres. Bulk electrical tests give the response of the whole device; electrical AFM modes map where it comes from. This note shows three complementary modes of the Nano-Observer II on memory devices, a dopant calibration structure and an oxide film: HD-KFM for surface potential, ResiScope for current and resistance, and Soft ResiScope for the same measurement without friction.

Quick answer

How to see p- and n-doped regions without damaging the device

Map the surface potential with Kelvin probe force microscopy (KPFM): no current flows through the device, and in HD-KFM™ the tip follows the surface in oscillating mode instead of scraping it. On an SRAM device, HD-KFM™ showed 30–50 mV between p-doped areas and n-doped channels and about 300 mV with the n-well, and revealed defective cells that do not show in the topography.

  1. Surface potential: HD-KFM™ records topography and potential together, on the second eigenmode of the cantilever; p- and n-doped regions appear as different potential levels.
  2. Which cells conduct: ResiScope™ on the same area, with the same cantilever and a 1 V sample bias. Soft ResiScope™ gives the same current and resistance without friction.
  3. Carrier concentration: potential values relate to it, but for quantitative values sMIM is better suited.

SRAM results: potential and current on the same area · Dopant profile on a SiC cross-section

Techniques

HD-KFM and ResiScope

HD-KFM measures the surface potential on the second eigenmode: the first eigenmode of the cantilever tracks the topography and the second, excited electrically at 350 to 400 kHz, tracks the potential, close to the surface, where the field is strongest (Figure 1). See lift-mode KPFM and HD-KFM compared.

Schematic comparison of lift-mode KFM and single-pass HD-KFM
Figure 1. Standard lift-mode KFM (left) and HD-KFM (right).

ResiScope is a contact mode that maps current and resistance over 10 orders of magnitude, from 50 fA (1 TΩ) to 1 mA (1 kΩ), without user intervention: a DSP selects the current-to-voltage amplifier in real time according to the resistance under the tip (Figure 2). A protective resistance limits the maximum current, minimizing local oxidation and cantilever self-heating. With a conventional fixed-range amplifier, insulating (pA) and conductive (µA–mA) regions of the same area cannot be measured at the same time.

Schematic of the ResiScope module with the Nano-Observer controller and smart module DSP
Figure 2. ResiScope: the smart module selects the amplifier in real time during the scan.

Results

SRAM: surface potential and current on the same area

Figure 3 shows the topography and the HD-KFM surface potential of an SRAM device (50 µm). The potential differs by only 30–50 mV between p-doped areas and n-doped channels, and by about 300 mV with the n-well. Some cells show defects in the potential map that do not appear in the topography. Potential values relate to carrier concentration, but for quantitative values sMIM is better suited.

SRAM device topography and HD-KFM surface potential, 50 micron scan
Figure 3. SRAM device, 50 µm: topography (left) and HD-KFM surface potential (right).

The same area was then measured in ResiScope without changing the set-up or the cantilever (Figure 4). Because the sample is biased (1 V), the current map also shows how the device performs: of the defects seen in Figure 3, one cell conducts normally while another shows no difference in current between p- and n-doped regions.

SRAM device ResiScope current and resistance maps, 50 micron scan, 1 V bias
Figure 4. SRAM device, same area, ResiScope at 1 V bias: current (left) and resistance (right).

Soft ResiScope gives the same quantitative current and resistance as ResiScope, without the friction of contact scanning. In Figure 5 the top of the image was scanned in Soft ResiScope and the bottom in standard ResiScope: drain, source and channel show the same conductivity in both.

SRAM topography and resistance, upper part in Soft ResiScope and lower part in standard ResiScope, with line profile
Figure 5. SRAM, one scan: Soft ResiScope (top) and standard ResiScope (bottom), with the resistance profile along the dashed line.

Your device

Measure your own semiconductor sample

Send a short description of the device and the measurement (surface potential, resistance, or both). The application team recommends a mode and can run test measurements on it.

Results

Dopant profile on a SiC cross-section

Figure 6 shows a cross-section of a silicon carbide (SiC) sample with regions of increasing carrier implant (a staircase structure). Each region is 500 nm wide; the resistance decreases from about 1 MΩ to 100 Ω across the steps. ResiScope tracks these several orders of magnitude (10² to 10⁶ Ω) in real time, without losing sensitivity. Polishing lines are visible in the topography.

SiC cross-section dopant staircase: topography, ResiScope resistance map and resistance profile from 10^6 to 10^2 ohm
Figure 6. Progressive dopant concentration in SiC, ResiScope: topography (top), resistance (middle) and resistance cross-section (bottom), from ~10⁶ Ω to ~10² Ω.

Results

VO₂: conductivity of grains during heating

Vanadium dioxide (VO₂) has a semiconductor–metal transition near 68 °C, with large changes in electrical and optical properties. At room temperature (295 K), Soft ResiScope shows the grain structure in both topography and current (Figure 7): grain currents stay below 1 nA at 1 V bias and vary between about 300 and 650 pA from grain to grain.

VO2 film topography and Soft ResiScope current at room temperature
Figure 7. VO₂ film at room temperature, Soft ResiScope: topography (left) and current (right).

With the heating accessory, the sample was ramped from 25 to 50 °C at 0.1 °C/min (Figure 8). The position stays stable and the current of the VO₂ domains rises from about 100 pA to 6 nA. Because the amplifier gain is software-controlled, no set-up change is needed as the current grows by orders of magnitude, while variations of about 50 pA between grains remain visible.

VO2 film topography and Soft ResiScope current at 25 °C and at 50 °C with the heating accessory
Figure 8. VO₂ film with the heating accessory, Soft ResiScope: topography and current at 25 °C (left pair) and at 50 °C (right pair).

Experimental

Measurement conditions

InstrumentNano-Observer II with HD-KFM, ResiScope and Soft ResiScope; heating accessory for the VO₂ ramp
SRAM50 µm scans; HD-KFM and ResiScope on the same area with the same cantilever; 1 V sample bias in ResiScope
Dopant staircaseSiC cross-section, 500 nm wide implant regions, ResiScope
VO₂ANSCM-PT probe (Pt/Ir, AppNano); applied force 1.8 nN; lift between points 20 nm; 1 V bias; 295 K, then 25 → 50 °C at 0.1 °C/min

Summary

Conclusion

HD-KFM maps surface potential with the resolution of the topography, revealing doped regions and defects; ResiScope and Soft ResiScope measure current and resistance over the largest dynamic range without changing the set-up, on insulating and highly conductive areas alike, and Soft ResiScope avoids friction. Because these modes are switched by software on the Nano-Observer II, the same area is measured with each, linking potential, conduction and device performance. They are also compatible with MFM and sMIM.

Already have an AFM?

Run the same measurements on your AFM

HD-KFM™ and ResiScope™ also run on a Bruker MultiMode or Dimension, or an Agilent / Keysight AFM, with the Galaxy Dual Controller upgrade.

In this note

AFM modes used

FAQ

Frequently Asked Questions

How can I see p- and n-doped regions on a semiconductor device without damaging it?

Map the surface potential with Kelvin probe force microscopy (KPFM): no current flows through the device, and in HD-KFM™ the tip follows the surface in oscillating mode instead of scraping it. On an SRAM device, HD-KFM™ showed 30–50 mV between p-doped areas and n-doped channels and about 300 mV with the n-well, and revealed defective cells that do not show in the topography.

How is AFM used to characterize semiconductor devices?

Electrical AFM modes map the properties that define a device at the nanoscale: surface potential with HD-KFM (doped regions, junctions, defects), current and resistance with ResiScope (device response under bias, dopant profiles), and permittivity and carrier concentration with sMIM.

Can AFM distinguish p- and n-doped regions?

Yes. On an SRAM device, HD-KFM showed differences of 30–50 mV between p-doped areas and n-doped channels and about 300 mV with the n-well, and revealed defective cells that were not visible in the topography.

Can ResiScope measure dopant profiles?

Yes. On a SiC cross-section with steps of increasing carrier implant, 500 nm wide each, ResiScope tracked resistances from about 100 Ω to 1 MΩ in real time, without changing the amplifier set-up.

Do HD-KFM and ResiScope require different set-ups?

No. On the Nano-Observer II the two modes are switched by software, with the same cantilever and without changing the set-up, so the same area is measured with both.

What is the advantage of Soft ResiScope on semiconductors?

It gives the same quantitative current and resistance as ResiScope, but without the friction of contact scanning, which limits damage. A scan of an SRAM measured half in Soft ResiScope and half in ResiScope showed the same results.

Can conductivity be followed during a temperature ramp?

Yes. With the heating accessory, Soft ResiScope followed the grains of a VO₂ film from 25 to 50 °C (0.1 °C/min); the current increased from about 100 pA to 6 nA with no amplifier change and stable position.

Characterize your semiconductor samples

Tell us the device and what you need to measure: doping, junctions, leakage paths or surface potential. The application scientists behind our AFMs answer every message personally.